Efni P355NH stál og P460NH eru þrýstihylkisstálflokkar samkvæmt EN10028-3 staðlinum. P355NH stál er óblandað gæðastál, en P460NH stál er málmblönduð sérstál.

 

P355NH stál og P460NH stál í efnasamsetningu (steypugreining, %)

 

Einkunnir C hámark Si max Mn P max S max Al(mín) N hámark Cr hámark Cu max Mo max Nb hámark Ni max Ti max V max Nb+Ti+ V hámark
P355NH 0.18 0.50 1.10-1.70 0.025 0.010 0.020 0.012 0.30 0.30 0.08 0.05 0.50 0.03 0.10 0.12
P460NH 0.20 0.60 1.10-1.70 0.025 0.010 0.020 0.025 0.30 0.70 0.10 0.05 0.80 0.03 0.20 0.22

 

Vélrænir eiginleikar

 

Einkunn Þykkt mm Uppskeruþol ReH MPa mín. Togstyrkur MPa Lenging % mín.
P355NH Minna en eða jafnt og 16 355 490~630 22
16<> 345 490~630 22
40<> 335 490~630 22
60<> 315 470~610 21
100<> 305 460~600 21
150<> 295 450~590 21
P460NH Minna en eða jafnt og 16 460 570~730 17
16<> 445 570~720 17
40<> 430 570~720 17
60<> 400 540~710 -
100<> - - -

 

Umsóknir

 

P355NH:

  • Lágt-hitageymslurými: Geymar fyrir fljótandi gas, frystihylki (td LNG geymsla) vegna -50 gráðu höggþols.
  • Miðlungs-þrýstihylki: Jarðolíukljúfar, katlar og leiðslur sem starfa við minna en eða jafnt og 400 gráður.
  • Almennar framkvæmdir: Brýr, úthafspallar og þungar vélar sem krefjast jafnvægis styrks og suðuhæfni.

 

P460NH:

  • Hár-þrýstingur/há-hitakerfi: Kjarnakljúfar, gufuhverfla og leiðslur við minna en eða jafnt og 400 gráður.
  • Mikilvægar innviðir: Úthafspallar, djúp-leiðslur og þungar-vinnuvélar sem þurfa mikla styrkleika og tæringarþol.
  • Öfgalegt umhverfi: Súrt eða ætandi umhverfi (td H₂S-sem inniheldur olíu/gas) vegna Ni og Mo viðbóta.

 

Við getum útvegað P355NH stál og P460NH staðlaða stálplötuþykkt allt að 250 mm. Velkomið að hafa samband við okkur ef þú hefur áhuga á sveigjanlegu fínkorna burðarstáli okkar.

Óska eftir tilboði

 

Ef þú vilt fræðast meira um vörur GNEE geturðu sent tölvupóst áalloy@gneesteelgroup.com. Við erum meira en fús til að aðstoða þig.

 

Hverju jafngildir P460NH efni?

P460NH er álblendi gæðastál með hækkuðu hitastigi með stöðlum skilgreindum í EN 10028-3 og EN 10216-3. Það hefur togstyrk á bilinu 560-730 MPa, lágmarksþol 460 MPa og lágmarkslenging 16%. Jafngildar einkunnir eru m.a18G2 (GOST) og WStE460 (DIN).

 

Hver er munurinn á p355n og P355NH?

P355 N og P355 Nh eru bæði þrýstihylkisstál, en þau eru mismunandi í fyrirhugaðri notkun miðað við hitastig.P355 N er hannað fyrir stofuhitaþjónustu, en P355 Nh er sérstaklega fyrir notkun á háum hita, sem þýðir að það heldur styrk sínum og eiginleikum við hærra hitastig.

 

Hver er ávöxtunarstyrkur P355NH?

275-460 N/mm²

P355NH er staðlað stálflokkur með lágmarksflæðiþol upp á275-460 N/mm²og plötur eru fáanlegar á lager frá vöruhúsi okkar. (Samanlagt magn af níóbíum, títan og vanadíum ætti að vera 0,12% að hámarki.)

 

P355NH steel and P460NH

P355NH steel and P460NH

P355NH steel and P460NH

 

Einkunnir þrýstihylkjaplötur frá GNEE
ASTM ASTM A202/A202M ASTM A202 bekk A ASTM A202 bekk B    
ASTM A203/A203M ASTM A203 bekk A ASTM A203 bekk B ASTM A203 bekk D ASTM A203 bekk E
ASTM A203 bekk F      
ASTM A204/A204M ASTM A204 bekk A ASTM A204 bekk B ASTM A204 bekk C  
ASTM A285/A285M ASTM A285 bekk A ASTM A285 bekk B ASTM A285 bekk C  
ASTM A299/A299M ASTM A299 bekk A ASTM A299 bekk B    
ASTM A302/A302M ASTM A302 bekk A ASTM A302 bekk B ASTM A302 bekk C ASTM A302 bekk D
ASTM A387/A387M ASTM A387 bekk 5 Class1 ASTM A387 bekk 5 Class2 ASTM A387 11. flokkur flokkur 1 ASTM A387 bekk 11 Flokkur 2
ASTM A387 bekk 12 Flokkur 1 ASTM A387 bekk 12 Flokkur 2 ASTM A387 bekk 22 Flokkur 1 ASTM A387 bekk 22 Flokkur 2
ASTM A515/A515M ASTM A515 bekk 60 ASTM A515 bekk 65 ASTM A515 bekk 70  
ASTM A516/A516M ASTM A516 bekk 55 ASTM A516 bekk 60 ASTM A516 bekk 65 ASTM A516 bekk 70
ASTM A517/A517M ASTM A517 bekk A ASTM A517 bekk B ASTM A517 bekk E ASTM A517 bekk F
ASTM A517 bekk P ASTM A517 bekk J    
ASTM A533/A533M ASTM A533 bekk A flokkur 1 ASTM A533 bekk B flokkur 1 ASTM A533 bekk C flokkur 1 ASTM A533 D flokkur 1
ASTM A533 bekk A flokkur 2 ASTM A533 bekk B flokkur 2 ASTM A533 bekk C flokkur 2 ASTM A533 bekk D flokkur 2
ASTM A533 bekk A flokkur 3 ASTM A533 bekk B flokkur 3 ASTM A533 bekk C Class3 ASTM A533 D flokkur 3
ASTM A537/A537M ASTM A537 flokkur 1 ASTM A537 flokkur 2 ASTM A537 flokkur 3  
ASTM A612/A612M ASTM A612      
ASTM A662/A662M ASTM A662 bekk A ASTM A662 bekk B ASTM A662 bekk C  
EN EN10028-2 EN10028-2 P235GH EN10028-2 P265GH EN10028-2 P295GH EN10028-2 P355GH
EN10028-2 16MO3      
EN10028-3 EN10028-3 P275N EN10028-3 P275NH EN10028-3 P275NL1 EN10028-3 P275NL2
EN10028-3 P355N EN10028-3 P355NH EN10028-3 P355NL1 EN10028-3 P355NL2
EN10028-3 P460N EN10028-3 P460NH EN10028-3 P460NL1 EN10028-3 P460NL2
EN10028-5 EN10028-5 P355M EN10028-5 P355ML1 EN10028-5 P355ML2 EN10028-5 P420M
EN10028-5 P420ML1 EN10028-5 P420ML2 EN10028-5 P460M EN10028-5 P460ML1
EN10028-5 P460ML2      
EN10028-6 EN10028-6 P355Q EN10028-6 P460Q EN10028-6 P500Q EN10028-6 P690Q
EN10028-6 P355QH EN10028-6 P460QH EN10028-6 P500QH EN10028-6 P690QH
EN10028-6 P355QL1 EN10028-6 P460QL1 EN10028-6 P500QL1 EN10028-6 P690QL1
EN10028-6 P355QL2 EN10028-6 P460QL2 EN10028-6 P500QL2 EN10028-6 P690QL2
JIS JIS G3115 JIS G3115 SPV235 JIS G3115 SPV315 JIS G3115 SPV355 JIS G3115 SPV410
JIS G3115 SPV450 JIS G3115 SPV490    
JIS G3103 JIS G3103 SB410 JIS G3103 SB450 JIS G3103 SB480 JIS G3103 SB450M
JIS G3103 SB480M      
GB GB713 GB713 Q245R GB713 Q345R GB713 Q370R GB713 12Cr1MoVR
GB713 12Cr2Mo1R GB713 13MnNiMoR GB713 14Cr1MoR GB713 15CrMoR
GB713 18MnMoNbR      
GB3531 GB3531 09MnNiDR GB3531 15MnNiDR GB3531 16MnDR  
DIN DIN 17155 DIN 17155 HI DIN 17155 HII DIN 17155 10CrMo910 DIN 17155 13CrMo44
DIN 17155 15Mo3 DIN 17155 17Mn4 DIN 17155 19Mn6